Silvestre Moreno (Outeiro de Rei)

Silvestre Moreno (Outeiro de Rei)
Other names
Moreno bóveda
Description

Textura panalotriomórfica inequigranular de tamaño de grano medio

Chromatic range
Ocher
Petrographic examination
Two-mica granite
Clasificación petrográfica Le Maitre
Monzogranite
image/svg+xml
Friol
Pena das vestas (Áridos H Carballido SL)
UNE-EN 1936 Apparent density 2560 kg/m3
Open porosity 3.2 %
UNE-EN 13755 Water absorption at atmospheric pressure
Mean value 1.1 %
Higher Expected Value (EH) 1.2 %
UNE-EN 14157 Abrasion resistance
Valor medio de la anchura de la huella 17.4 mm
Higher Expected Value of groove´s width 17.8 mm
UNE-EN 12372 Flexural strength
Mean value 9.6 MPa
Low expected value (EL) 7.3 MPa
UNE-EN 12371 Frost resistance, 56 cycles
Decreased flexural strength 1.5 %
Valor medio de resistencia a flexión 9.5 MPa

Granite has been tested in the CTG laboratory. The results of these tests are only related to the samples tested.